免研磨分散型彩色顏料參數(shù)表
型號 | 名稱 | 索引號 | 耐熱 | PH 值 | 吸油量 | 耐光 | 抗?jié)B色 | 耐酸 | 耐堿 | 耐醇 | 耐水 | 耐油 | 耐酯 | 耐苯 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS15Y | 永固黃 | PY13 | 200 | 6~8 | ≤55 | 5~6 | 5 | 5 | 5 | 5 | 4 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS14Y | 金黃 | PY83 | 220 | 6~8 | ≤45 | 6~7 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS16Y | 檸檬黃 | PY3 | 180 | 6~8 | ≤40 | 7~8 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS07R | 寶紅 | PR57:1 | 200 | 7~9 | ≤55 | 6~7 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS09R | 永固紅 F5RK | PR170 | 200 | 6~8 | ≤45 | 6~7 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
H-505 | 桃紅 | PR122 | 250 | 6~7 | ≤50 | ≧8 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS13B | 群青 | PB29 | 350 | 6~8 | ≤40 | 7~8 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS05B | 酞菁蘭 | PB15:3 | 220 | 6~8 | ≤55 | ≧8 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
FS07G | 酞菁綠 | PG7 | 200 | 6~8 | ≤55 | 7~8 | 5 | 5 | 5 | 5 | 5 | 5 | 5 | 5 |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
免研磨分散型顏料特點(diǎn):高光澤、低吸油量、易分散、無需研磨
主要應(yīng)用領(lǐng)域:涂料、油墨、皮革、電池

產(chǎn)品說明:
本產(chǎn)品在理想的分散狀態(tài)下即能迅速的達(dá)到較高的色濃度,不需較強(qiáng)的外力(例如研磨),所以其生產(chǎn)制程與傳統(tǒng)生產(chǎn)工藝有諸多不同,在使用本產(chǎn)品時請依本說明書進(jìn)行。
使用方法:
步驟 | 原料 | 制程 | 備註 |
NO. 1 | 溶劑/分散劑/樹脂
| 工序:攪拌 設(shè)備:攪拌機(jī) 參數(shù):600RPM*20分鐘
| 專用分散劑,加入樹脂後分散均勻 |
NO. 2 | 色粉 | 工序:攪拌 設(shè)備:攪拌機(jī) 參數(shù):(≥1500RPM)*(≥30分鐘)
| 細(xì)度≤10um |
NO.3 | 其他 | 工序:攪拌 設(shè)備:攪拌機(jī) 參數(shù):自定
|
依配方設(shè)定添加
|
重要說明:
鑒於顏料功能的局限性及用戶要求的多樣性,使用前請按自身的要求,嚴(yán)格試驗(yàn)顏料的適用
性及最終產(chǎn)品的穩(wěn)定性。以上資料僅供參考,本公司不作法律擔(dān)保及不負(fù)任何法律責(zé)任。
注意事項(xiàng):
請?jiān)谕L(fēng)乾燥條件下保存。
建議配方:(實(shí)驗(yàn)測試用)粉量:15%
丁酯:33克
分散劑:4.5克(略攪,溶於丁酯內(nèi))
樹脂:90克
------600RPM攪拌10分鐘,分散均勻
分散型顏料:22.5克
------1500RPM攪拌30分鍾